GEMYSKE GEARSTALLING
incoloy 625 coiled tubing capillary tubing
C | Cr | Ni | Fe | Mn | Si | Mo | Co | P | S | Ti | Nb + Ta | Al |
---|---|---|---|---|---|---|---|---|---|---|---|---|
≤ 0.1 | 20 – 23 | ≥ 58 | ≤ 5 | ≤ 0,5 | ≤ 0,5 | 8 – 10 | ≤ 1* | ≤ 0,015 | ≤ 0,015 | ≤ 0,4 | 3.15 – 4.15 | ≤ 0,4 |
(massa%)
* As bepaald
ASTM B444, ASME SB444, AMS 5581
Per ASTM B444, ASME SB444, AMS 5581
Betingst | Treksterkte | Yield sterkte | Ferlinging |
minimum, ksy | minimum, ksy | minimum, % | |
Klasse 1 | 120 | 60 | 30 |
Klasse 2 | 100 | 40 | 30 |
* Hegere sterkte eigenskippen kinne wurde levere yn 'e kâld ferhurde tastân.
incoloy 625 coiled tubing capillary tubing
70°F | 200°F | 400°F | 600°F | 800°F | 1000°F | ||
---|---|---|---|---|---|---|---|
Tichtheid | lbs/yn3 | 0.305 | - | - | - | - | - |
Termyske útwreiding | X10-6/°F | - | 7.1 | 7.3 | 7.4 | 7.6 | 7.7 |
Elastyske modulus | 103 ksj | 30.1 | 29.6 | 28.7 | 27.8 | 26.9 | 25.7 |
Poisson Ratio | - | 0.278 | 0.28 | 0.286 | 0.29 | 0.295 | - |
Warmtegelieding | Btu-in/h·ft2·°F | 68 | 75 | 87 | 98 | 109 | 139 |
Spesifike waarmte | Btu/lb·°F | 0.098 | 0.102 | 0.109 | 0.115 | 0.122 | 0.118 |
Yield sterkte | ksi | 70 | 68 | 63 | 60 | 59 | 34 |
Treksterkte | ksi | 140 | 134 | 130 | 129 | 129 | 88 |
incoloy 625 coiled tubing capillary tubing
PROCESSBESKRIJVINGStiel MakingElectric Arc Furnace folge troch Vacuum Oxygen Decarburization (VOD) of Argon Oxygen Decarburization (AOD). Pipe Making Konvinsjonele Seamless Cold Finished Pipe en Tube Manufacturing Processes. Heat TreatmentCannot wurde ferhurde troch waarmte behanneling.Kin wurde levere yn 'e annealed, oplossing annealed of kâld ferhurde steat.De hegere sterkte annealed betingst wurdt typysk brûkt yn tsjinsten oant 1100 ° F, wylst de oplossing annealed betingst wurdt brûkt yn applikaasjes boppe 1100 ° F.